fireclay brick
|
|
|
|
|
|
|
|
|
|
N1-1 |
N2-1 |
N3-1 |
Spec |
Typical |
Spec |
Typical |
Spec |
Typical |
Chemical Analysis (%) |
Al2O3 |
38¡Ü |
40 |
32¡Ü |
35 |
31¡Ü |
33 |
Fe2O3 |
2.5¡Ý |
1.9 |
2.5¡Ý |
2.0 |
2.5¡Ý |
2.0 |
Refractoriness (SK) |
34¡Ü |
34 |
33¡Ü |
33 |
32¡Ü |
32 |
Bulk Density |
2.00¡Ü |
2.25 |
1.95¡Ü |
2.20 |
1.90¡Ü |
2.15 |
Apparent Porosity (%) |
24¡Ý |
19 |
24¡Ý |
19 |
26¡Ý |
19 |
Cold Crushing Strength |
200¡Ü |
400 |
200¡Ü |
350 |
200¡Ü |
350 |
(Kg/cm2) |
Thermal Expansion (%) |
- |
0.56 |
- |
0.52 |
- |
0.53 |
at 1000¡æ |
Permanent Linear Change (%) |
- |
0.5 |
- |
0.5 |
- |
1350¡æ 0.5 |
at 1400¡æ ¡Á 2Hrs |
Refractoriness under Load |
- |
1,370 |
- |
1,360 |
- |
1,360 |
(2Kg/cm2, T2¡æ) | |
|
|
|